Table 1 Summary of the PVC and PP/Talc batches that have been milled in the Dispermat Ball Mill

From: Protocol for the production of micro- and nanoplastic test materials

Batch

Mass

Mass ZrO2 beads (1 mm)

Milling time

Conditions

PVC_BI

72 g

1100 g

20 h @ 6000 rpm

RT, ethanol

PVC_BII

72 g

1100 g

20 h @ 6000 rpm

RT, ethanol

PVC_BIII

90 g

1200 g

20 h @ 6000 rpm

RT, ethanol

PVC_BVI

60 g

1000 g

25 h @ 3000 rpm

RT, 1-propanol

PP/Talc_BV

50 g

1130 g

65 min @ 2000 rpm

LN2, 1-propanol

PP/Talc_BVII

32 g

600 g

60 min @ 2000 rpm

LN2, 1-propanol

PP/Talc_BVIII

30 g

600 g

60 min @ 3000 rpm